5倍,最低不宜小于0.5Mpa,并保持试验压力2h和满足设计的特殊要求。每当压力降落0.02Mpa时,则应向管内补水。为保持管内压力所增补的水为漏水量的计算值。若漏水量不超过规定的允许值,强度试验即为合格。容许漏水量见表9-4、表9-5.试压时的有关规定:对于粘结连接的管道须在安装完毕48h后才能进行试压。②管道的强度试压工作应在沟槽回填至管顶以上0.6m并至少48h后才能进行。③试压管段上的三通、弯头特别是管端的盖堵的支撑要有足够的稳定性。若采用混凝土结构的止推块,试压前要有充分的凝固时间,使其达到规定的抗压强度。④试压时,向管道注水的同时要排掉管内的空气,水必须慢慢地进入管道防止发生气锤和水锤。表9-4UPVC给水管道容许漏水量管径(mm)容许漏水量(L·min﹣1·km﹣1)管径(mm)容许漏水量(L·min﹣1·km﹣1)粘接连接橡胶圈连接粘接连接橡胶圈连接63~7590~110125~140160~1800.20~0.240.26~0.280.35~0.380.42~0.500.30~0.500.60~0.700.90~0.951.05~1.20200225~2502803150.560.700.800.851.401.551.601.70表9-5UPVC排水管道允许渗水量公称直径(mm)双壁波纹管直臂管内径(mm)允许渗水量{m3·(24h·km)﹣1}内径(mm)允许渗水量{m3·(24h·km)﹣1}110125160200250315400450500630971071351722162703403834325400.450.490.620.790.991.241.561.761.992.48103.6117.6150.6188.2235.4296.6376.6-470.8593.20.480.540.690.871.081.361.73-2.172.73